Content on this page supplied from the web site of Jim Lux
Surface Preparation for Epoxy Bonding
Proper surface preparation before bonding with epoxies is essential. Here is a summary of prep
techniques taken in a larger part from "the Bell Jar".
Aluminum and Aluminum Alloys
- Degrease with trichloroethylene
- Dip in the following solution for 10 minutes:
3 parts sodium dichromate
20 parts water
10 parts 95% sulfuric acid
- Rinse in ambient tap water
- Rinse in hot (65-75 degrees C) distilled water
- Air dry
- Note: Some alloys, such as #360, only require one to three minute dip in the acid
dichromate.
Copper, Brass, and other Copper Alloys
- Degrease with trichloroethylene
- Dip in either of the two following solutions
6 parts ferric chloride
200 parts water
30 parts concentrated nitric acid (70%)
OR
25% ammonium persulfate for 1-2 minutes
- Rinse with distilled water and dry
Ferrous alloys other than Stainless
- Degrease with trichloroethylene
- Sandblast with 100 grit sand or etch in 15% hydrochloric acid (equal parts concentrated
hydrochloric acid and water) for 10 minutes. Etched surfaces should be rinsed immediately
and dried with hot air.
Freshly sandblasted or etched steel begins to rust immediately; therefore adhesive should be
applied as soon as the surface has been prepared.
Stainless Steel, Chromium
- Degrease with trichloroethylene
- Etch with concentrated hydrochloric acid for 15 minutes at room temperature OR with a
solution of
90 parts water
40 parts 96% sulfuric acid
0.2 parts Nacconol NR (National Aniline)
for 10 minutes at 65 degrees C followed by
90 parts water
15 parts 70% nitric acid
2 parts 48% hydrofluoric acid
- Rinse in hot distilled water and dry with hot air.
Zinc, Lead, Nickel, and Tin
- Degrease
- Abrade(sandblast)
- Degrease
Stone, Ceramics, Glass
- Degrease
- Wire Brush (for stone) and sandblast
- Rinse with water and dry
Polar Thermoplastics (Nylon, ABS, Polycarbonate, Acrylate)
- Degrease with trichloroethylene
- Abrade
- Degrease
Polyethylene, Polypropylene
- Degrease with trichloroethylene
- Oxidize by immersing in a solution:
7 parts sodium dichromate
10 parts water
150 parts concentrated sulfuric acid
for 10-15 minutes
- Rinse with hot distilled water
- Dry and coat with adhesive immediately
Thermoset plastics (Epoxies, Polyurethane, Polyester, Melamine, Phenolic)
- Degrease with acetone, MEK, or trichloroethylene
- Mechanically abrade (sandblast)
- Degrease
Copyright 1998, Jim Lux / epoxprep.htm / 5 Mar 1998 / Back to HV Home / Back to home page / Mail to Jim